Frozen food packaging must withstand two critical temperature challenges: the temperature drop process when the product enters the rapid freezing tunnel or cold storage after hot filling and sealing, and the prolonged negative temperature storage and subsequent temperature fluctuations during distribution. These two stages impose specific requirements on the low-temperature resistance of the film and the low-temperature strength of the heat-sealed areas.
Polyethylene-based heat-sealing layers exhibit excellent flexibility and sealing strength at room temperature. However, when the temperature drops below the glass transition temperature, molecular chain mobility is restricted, leading to increased material modulus and reduced elongation at break. If the proportion of linear polyethylene in the formulation is inappropriate or lacks toughening components, microcracks are prone to form at the sealed edges during folding, pressing, or drop impacts. Solutions include blending a certain proportion of ethylene-vinyl acetate copolymer with metallocene-catalyzed linear polyethylene. The vinyl acetate side chains increase molecular chain spacing and reduce crystallinity, enabling the heat-sealing layer to maintain extensibility even at sub-zero temperatures. Additionally, heat-sealing process parameters must be properly matched: sealing knife temperature, dwell time, and cooling temperature affect the cohesive strength of the seal and the density of the sealing interface. Excessive heat can cause degradation or necking of the inner resin layer, while insufficient heat results in inadequate peel force at the sealed interface.
In addition to the strength of the heat-sealed area itself, the root of the heat seal, which is the transition zone between the seal and the bag body, is a stress concentration point. In drop tests for heavier contents such as frozen dumplings and rice dumplings, cracks often originate at the heat-sealed root rather than the center of the seal. To address this, bag production typically employs rounded transition angles or widened heat-sealed margins, and the alignment accuracy of the vertical and horizontal sealing dies on the bag-making machine is adjusted to prevent seal misalignment that could lead to localized weakness.
Yantai Dongsheng Packaging conducted cold resistance modification ratio tests on the inner layer materials during the production of frozen bags, and verified the bag performance through dart impact and low-temperature drop tests. The bag-making process was set with a dedicated heat sealing parameter window, distinguishing the sealing conditions for stand-up zipper bags and three-sided vacuum bags based on bag type and thickness. Additionally, heat sealing strength and bending resistance were tested in each batch. For stand-up zipper bags, special attention was paid to reinforced sealing at the zipper and bag body junction to prevent the zipper root from becoming a starting point for cracking after freezing.
For users, when inspecting frozen packaging bags, in addition to visual checks for printing and dimensions, it is recommended to conduct sampling tests for heat-sealed peel strength after low-temperature freezing and single-corner suspension drop impact, simulating potential impacts during actual distribution. If the seal turns white and breaks without obvious fiber pulling, it often indicates insufficient heat-sealing temperature or inadequate low-temperature resistance of the inner layer; if the bag body has punctures while the seal remains intact, it suggests the need to adjust the thickness of the puncture-resistant layer or the nylon material selection. Incorporating such simulated tests into incoming material inspection can help prevent post-freezing bag breakage complaints from the outset.
Keep up with our latest newsletter.